MESIN EXTRUSION LAMINATING

By | 08.21 Leave a Comment
MESIN EXTRUSION LAMINATION


PROSES  PRODUKSI  MESIN EXTRUSION.

Komposisi bahan proses.= OPP.20 micron, /tinta + resin PP.20 micron
Speed mesin = 60.
Speed  R P M = 3250 – s/d – 3300.
Chiller colling roll = 25 C – s/d – 28 C.
  1. Bahan proses produksi resin PP. Di oven dulu terus masukan ke hopper.
  2. Setting heatter panas sesuai bahan resin yang digunakan proses produksi.
  3. Lamanya panas titik lebur bahan resin PP.  -/ +  2  jam
  4. Heatter  adapter setting panas. A.1 = 260 C / A.2 = 260 C.
  5. SETTING HEATTER LEHER.C.1 = 170.C/ C.2 = 200.C/ C.3 = 230.C/ C.4 = 260. C
  6. SETTING HEATTER KEPALA.D.1 = 255.C/ D.2 = 260.C/ D.3 = 260.C/ D.4 = 260.C/ D.5 = 255.C.
  7. Titik lebur resin PP/PE lamanya + 3 jam.

MESIN EXTRUSION LAMINATION TANDEM


PROSES UNTUK PRODUKSI
Komposisi bahan proses produksi.= OPP.20 mic/ printing + resin  PE.20 micron.
Speed mesin = 60  -> Speed  RPM. = 3250 s/d 3300 -> Ciller = 25 -.C s/d – 28.C
Resin PE masukan ke HOPER setelah resinnya di oven supaya tidak lembab.
Setting PE sesuai panasnya jenis resin yang dipakai untuk proses produksi.
Untuk setting heatter resin PE  titik lebur panasnya heatter lamanya -/ +  2 jam.
Setting heatter adapter. =  A.1 = 360.C / A.2 = 360.C
SETTING HEATTER LEHER.
C.1 = 180. C./ C.2 = 250.C./ C.3 = 335.C./ C.4 = 360.C.
SETTING HEATTER KEPALA.
D.1 = 355.C/ D.2 = 360.C/ D.3 = 360.C/ D.4 = 360.C/ D.5 = 355.C